Defects and preventive measures of stamping and stretching parts
Time : 2023-08-30 Click count : 2709

1. Reasons for waste generation:

A. Poor quality of raw materials;

B. Improper installation, adjustment, and use of molds;

C. The worker did not feed the strip correctly along the positioning or did not ensure that the strip was fed with a certain gap;

D. Due to long-term use of the mold, there may be changes in gaps or wear on the working and guiding components of the mold;

E. Due to prolonged impact and vibration, the fastening parts of the mold become loose, causing a relative change in the installation position of the mold;

F. The operator's negligence did not follow the operating procedures.


2. The main measures to prevent waste are:

A. Raw materials must meet the specified technical conditions (strictly inspect the specifications and brands of raw materials, and conduct laboratory tests on workpieces with high requirements for dimensional accuracy and surface quality when conditions permit)

B. All aspects specified in the process specifications should be strictly followed comprehensively;

C. The tools and equipment used, such as presses and molds, should ensure that they work under normal working conditions;

D. Establish a strict inspection system during the production process, which requires a thorough inspection of the first stamped part. Only after passing the inspection can they be put into production. At the same time, inspection should be strengthened, and accidents should be dealt with in a timely manner;

E. Adhere to the civilized production system, for example, workpieces and blanks must be transported using appropriate workstation equipment, otherwise the surface of the workpiece will be crushed and scratched, affecting the surface quality of the workpiece;

F. During the stamping process, the cleanliness of the mold cavity should be ensured, and the orderly arrangement of workpieces after processing in the workplace should be neat.


3. Causes of burrs on punched parts

A. The punching gap is too large, too small, or uneven;

B. The cutting edge of the working part of the mold becomes dull;

C. Due to long-term vibration impact, the centerlines of the convex and concave molds change, and the axes do not coincide, resulting in one-sided burrs.

measures:

1) Ensure the machining accuracy and assembly quality of convex and concave molds, ensure the verticality of convex molds, withstand lateral pressure, and ensure the rigidity of the entire mold;

2) When installing the convex mold, ensure that the gap between the convex mold and the concave mold is correct, and firmly install the convex mold and the concave mold on the mold fixing plate. The end faces of the upper and lower molds should be parallel to the worktable of the press.

3) The requirements for the press include good rigidity, minimal elastic deformation, high track accuracy, and high parallelism between the pad and slider;

4) Require the pressure machine to have sufficient punching force.

The allowable height of burrs on the cut surface of punched parts

Punched sheet thickness>0.3>0.3-0.5>0.5-1.0>1.0-1.5>1.5-2.0

New trial mold burr height ≤ 0.015 ≤ 0.02 ≤ 0.03 ≤ 0.04 ≤ 0.05

The allowable burr height in production is ≤ 0.05 ≤ 0.08 ≤ 0.10 ≤ 0.13 ≤ 0.15


4. Reasons for warping and deformation of punched parts:

There are clearance forces and reaction forces on a straight line that do not generate torque. When the gap between the punch and the die is too large, the edge of the die has a conical shape, or when the contact area between the ejector and the workpiece is too small, warping deformation will occur

measures:

A. Reasonably choose the punching gap;

B. In the mold structure, a certain amount of pressure is required to increase the plane contact between the pressing plate (or support plate) and the pressing plate;

C. Check the concave die blade. If a reverse taper is found, the cutting edge of the die must be trimmed correctly.

D. When the shape of the punched part is complex and there are many inner holes, if the cutting force is uneven, the pressing force will increase. Before punching, press the strip tightly or use a high-precision press to punch it.

E. Before punching the sheet metal, it should be leveled. If the warping cannot be removed, the punched workpiece can be re leveled using a leveling mold.

F. Regularly clean the dirt inside the mold cavity, lubricate the surface of the thin sheet material, and install oil vent holes on the mold structure.


5. During punching, the accuracy of the outer edge and inner hole of the punched part decreases, and the size changes.

reason:

The position of positioning pins, blocking pins, etc. has changed or worn out excessively;

The operator's carelessness caused the material to move back and forth during feeding;

The dimensional accuracy of the strip material is low, too narrow and too wide, making it difficult to deliver to the designated location. If the strip material moves back and forth in the guide plate, the punching hole of the workpiece will have a significant deviation from the front and rear positions of the outer shape.


6. Reasons for non-conforming bending dimensions and shapes of parts

A. The rebound of the material causes the product to be unqualified

Measures to reduce rebound:

Choose stamping materials with stable mechanical properties, high elastic modulus, and low yield point;

Add calibration program and use calibration bending instead of free bending;

Before bending, the material should be annealed to soften the cold work hardened material before bending into shape;

If there is shape deformation during stamping, it is difficult to remove; Then change or adjust the slope of the convex and concave molds, and the gap between the convex and concave molds should be equal to the minimum material thickness.

Increase the contact area between the concave mold and the workpiece, and reduce the contact area between the convex mold and the workpiece.

Reduce the impact of rebound by overcorrecting.

B. If the locator is worn and deformed, causing inaccurate positioning of the strip, a new locator must be replaced.

C. In non guided bending molds, improper adjustment of the bottom dead center position of the press slide during adjustment on the press can also result in the shape and size of the bent part being non-conforming.

D. If the pressing device of the mold malfunctions or does not work at all, it is necessary to readjust the pressing force or replace the pressure spring to make it work normally.


7. Cracks appear at the bending part of the bent part (the internal stress in the bending deformation zone exceeds the material strength limit)

A. Removing burrs outside the curved area can lead to stress concentration in that area,

1) Reduce bending deformation

2) Remove burrs from the area

3) Place the side with burrs inside the curved area

B. When bending workpieces, it is best to make the bending direction perpendicular to the fiber direction (rolling direction) of the material.

C. The bending radius should not be too small, and if the quality allows, the fillet radius should be increased as much as possible.

D. The surface of the bent blank should be smooth, without obvious protrusions or scars.

E. Intermediate annealing process is used to remove internal stress during bending, and softening bending rarely produces cracks.

F. When bending, larger bending parts must be coated with lubricant to reduce friction during bending.


8. Deviation of bent parts during bending process

During the bending process, when the blank slides along the surface of the concave mold, it will experience frictional resistance. If the frictional resistance on both sides of the blank is significantly different, the blank will move towards the side with greater frictional resistance.

measures:

1) Asymmetric bending parts are formed by symmetrical bending (single-sided bending parts are cut after two symmetrical bends)

2) Add an elastic compression device on the bending mold to compress the billet and prevent it from moving during bending.

3) Utilize internal holes and external positioning forms to ensure accurate positioning.


9. Reasons and solutions for surface scratches on curved parts.

A. When continuously bending soft materials such as copper and aluminum alloys, metal particles or slag are prone to adhere to the surface of the working area, causing significant scratches on the parts. At this time, it is necessary to carefully analyze and study the shape and lubricating oil of the working parts, and it is best to avoid particles and slag on the blank, which can cause scratches.

B. When the bending direction is parallel to the rolling direction of the material, cracks will appear on the surface of the workpiece, reducing the surface quality of the workpiece. When two or more parts are bent, ensure that the bending direction is as close as possible to the rolling direction.

C. When the burr surface is bent as the outer surface, the parts are prone to cracking and scratching; Therefore, the burr surface should be considered as a curved inner surface.

D. The fillet radius of the concave mold is too small, and there are impact marks on the curved part. Polishing the concave mold and increasing the fillet radius of the concave mold can avoid wear on bent parts.

E. The gap between the convex and concave molds should not be too small, otherwise it will cause thinning and wear. Regularly check the changes in mold clearance during stamping.

F. If the depth of the convex mold entering the concave mold is too large, there may be scratches on the surface of the part. Therefore, while ensuring that it is not affected by rebound, the depth of the convex mold entering the concave mold should be appropriately reduced.

G. In order to meet the precision requirements of the parts, bottom pressing bending molds are often used. When bending, the springs, locating pin holes, support plates, and return holes on the pressing plate will be pressed into indentations and should be adjusted.


10. What is the reason for the change in the position of the blank hole during bending? How to exclude

A. The position and size of the hole are incorrect, resulting in thinning due to bending and stretching

Measures: Strictly control the bending radius, bending angle, and material thickness; Trim the neutral layer of the material so that the depth of the convex mold entering the concave mold and the depth of the convex and concave molds are appropriately consistent.

B. Reasons for non concentric holes

1) Insufficient bending height. 2) The blank slides. 3) Rebound. 4) The curved plane exhibits undulations.

measures:

1) Ensure the correct left and right bending height.

2) Correct the worn positioning pins and plates.

3) Reduce rebound and ensure the parallelism and flatness of the two curved surfaces.

4) Change the process route, first bend and correct before punching.

C. The bending curve is not parallel to the centerline of the two holes, and the part with a bending height less than the minimum bending height shows an outward opening shape after bending.

measures:

1) When bending, the minimum bending height H (H ≥ R 2t t material thickness R bending radius) should be ensured.

2) Change the shape of the processed parts and remove parts with a bending height less than the minimum without affecting their use.

D. Holes near curved lines are prone to deformation.

measures:

1) When designing bent parts, ensure that the edge distance X from the bent part to the hole is greater than a certain value X ≥ (1.5-2.0) t t t of the bent sheet thickness.

2) Designing auxiliary holes in the bending area to absorb bending deformation stress can prevent hole deformation near the bending curve. Generally, the scheme of bending first and punching later is adopted.


11. After bending, the bent parts show significant thinning

A. The bending radius is too small relative to the plate thickness value (r/t>3 right angle bending). Generally, increasing the bending radius is used.

B. Multi angle bending makes the bent part thinner and larger. In order to reduce thinning, the single angle multi process bending method should be used as much as possible.

C. When using a pointed convex mold, the convex mold enters the concave mold too deeply, significantly reducing the thickness of the bent part.


12. Reasons and prevention of flange wrinkling during deep drawing process of deep drawn parts

reason:The edge pressure on the flange is too small to resist excessive tangential compressive stress; And it causes tangential deformation, resulting in the formation of folds after losing stability. Thinner materials are also prone to wrinkle formation.

measures:Increase the edge pressure of the edging ring and appropriately increase the thickness of the material.


13. Reasons and prevention of wall cracking in deep drawn parts

reason:

A. Excessive radial tensile stress of the material during stretching;

B. The radius of the concave mold fillet is too small,

C. Poor lubrication during deep drawing;

D. The plasticity of raw materials is poor.

measures:

1) Reduce the edge pressure.

2) Increase the fillet radius of the concave mold.

3) Proper use of lubricants.

4) Choose materials with better performance or add annealing processes in the workshop.


14. The bottom of the deep drawn part is cracked by pulling

The reason is that the fillet radius of the concave mold is too small, which causes the material to be cut. (Usually occurring in the early stage of deep drawing) Increasing the fillet radius of the concave die reduces the surface roughness of its smooth transition, usually Ra<0.2 μ m.


15. The edges of the deep drawn parts are uneven and wrinkled.

reason:The blank and the center of the convex concave die are not in a straight line or the material thickness is uneven. The radius of the concave die corner is uneven with the gap between the convex concave die (if the radius of the concave die corner is too large, the edge pressing ring and the edge pressing ring will separate in the final stage of deep drawing, and the material that does not cross the corner cannot be pressed into the edge pressing ring and wrinkled before being pulled into the concave die to form mouth edge wrinkles).

measures:Repositioning the die, before putting it into production, adjust the fillet radius of the concave die and the clearance between the convex and concave dies to make them uniform in size (reducing the fillet radius of the concave die or using an arc-shaped edge pressing ring device can remove wrinkles)


16. Reasons and preventive measures for wrinkling at the waist during deep drawing of conical or hemispherical parts:

reason:At the beginning of deep drawing, most of the material is in a suspended state, with too little edge pressure, too large fillet radius of the die, or excessive use of lubricant. The radial tensile stress decreases, and the material loses stability under tangential compressive stress, resulting in wrinkles.

measures:Increase the edge pressure or adopt a rolled rib structure, reduce the fillet radius of the concave die or slightly increase the material thickness.


17. Reasons and preventive measures for drawing marks on the surface of deep drawn parts

reason:

A. If there are sharp scratches on the surface of the convex or concave mold, resulting in corresponding tensile marks on the surface of the workpiece, the surface should be polished or buffed.

B. The gap between the convex and concave molds is too small or uneven, causing scratches on the surface of the workpiece during deep drawing. At this time, the gap between the convex and concave molds should be adjusted until it is suitable.

C. The concave die has a rough rounded surface, and the workpiece surface is scratched during stretching. At this point, the radius of the rounded corners of the concave mold should be polished and smoothed.

D. During stamping, impurities are mixed into the working surface or material surface of the die due to uncleanliness, which damages the surface of the workpiece. Therefore, the surface of the convex and concave molds must always be kept clean during material pulling, and the blank must be wiped before pulling;

E. When the hardness of the convex and concave molds is low, metal shavings will adhere to their surfaces, and there will also be stretch marks on the surface of the deep drawn workpiece. Therefore, in addition to increasing the hardness of the convex concave die surface, even if the remaining metal waste is removed, the surface of the convex concave die should always be inspected.

F. Poor quality lubricants can also increase the surface roughness of deep drawn workpieces. In this case, lubricants suitable for deep drawing processes should be used, and if necessary, the lubricant should be filtered before use. Thus preventing impurities from entering and damaging the surface of the workpiece.


18. What is the reason for the unevenness of the straight wall of the deep drawn part?

reason:

A. There are no ventilation holes designed and manufactured on the convex mold, so the surface of the convex mold will deform due to compressed air, resulting in unevenness. In this case, ventilation holes must be added.

B. The rebound of the material can also cause unevenness on the surface of the deep drawn workpiece, and finally, a shaping process needs to be added.

C. The gap between the convex and concave molds is too large, making it difficult to flatten during deep drawing. At this time, the gap must be uniformly adjusted.

News Related news
欧美爱爱视频| 亚洲精品va| 91影院在线免费观看视频| 在线观看免费观看在线91| 日韩电影中文字幕一区| 欧洲一级精品| 欧美性受xxxx黑人| 欧美一区二区三区在| av在线加勒比| 日本一二区免费| 蘑菇福利视频一区播放| 国产婷婷在线观看| 国产美女久久久久| 久久黄色精品视频| 亚洲欧美精品午睡沙发| 99综合精品久久| 亚洲精品欧美在线| 五月婷婷婷婷婷| 亚洲欧美视频| 亚洲妇女无套内射精| 99久久精品费精品国产风间由美| 日本成人在线免费视频| 日本女优在线视频一区二区| 一本在线免费视频| 国内精品久久久久久久97牛牛| 日本少妇在线观看| 成人免费网站在线观看视频| 欧美三级在线观看视频| 日韩av懂色| 成人久久电影| 黑人精品欧美一区二区蜜桃| 国产精品免费人成网站| 日本大香伊一区二区三区| 亚洲色图17p| 亚洲一区二区三区视频| 黑人糟蹋人妻hd中文字幕| 黄色免费一级视频| 色婷婷激情五月| 日本我和搜子同居的日子高清在线| 99久久精品免费观看国产| 伊人春色精品| 丁香激情综合国产| 777亚洲妇女| 国产精品极品美女在线观看免费| 在线视频一二三区| 极品蜜桃臀肥臀-x88av| 男女猛烈无遮挡午夜视频| 日本在线视频1区| 警花av一区二区三区| 久久精品国产免费| 欧美性色欧美a在线播放| 97超碰色婷婷| 凹凸国产熟女精品视频| 日韩av女优在线观看| 日皮视频在线免费观看| 日本黄色免费在线| 久久九九电影| 在线亚洲精品福利网址导航| 国产不卡av在线| 国产福利在线免费| 国产精品久久久国产盗摄| 激情四房婷婷| 欧美巨大xxxx| 国产亚洲综合av| 国产一区二区三区三区在线观看| 日本一区免费观看| 性欧美疯狂猛交69hd| 日本老妇乱子| 久久久久黄色| 国产传媒日韩欧美成人| 精品美女被调教视频大全网站| 国产a一区二区| 国产激情在线免费观看| 欧美性xxxx交| 亚洲第一影院| 国产精品1024| 日韩乱码在线视频| 亚洲免费视频一区| 国产午夜精品无码一区二区| 色视频网站在线| 精品福利一区| 亚洲欧美激情小说另类| 国产成人jvid在线播放| 麻豆免费在线观看视频| 性欧美最新另类| 欧美最新精品| av在线播放不卡| 九九热精品视频国产| 黄色免费观看视频网站| 国产精品久久久久精| 日本视频在线观看| 日韩国产高清影视| 精品五月天久久| 国产原创中文在线观看 | 一区二区精品免费| 免费能直接在线观看黄的视频| 成人豆花视频| 亚洲欧洲美洲综合色网| 国产在线视频2019最新视频| 国产午夜精品视频| 欧美激情精品久久久久久黑人| 99视频在线视频| 在线观看精品自拍视频| 亚洲成人高清| 亚洲美女偷拍久久| 国产精品视频入口| 自拍偷拍欧美亚洲| 看女生喷水的网站在线观看| 激情欧美日韩一区二区| 九九热精品视频国产| www.88av| 亚洲精华国产| 视频一区二区不卡| 日韩在线观看免费高清完整版| 杨幂毛片午夜性生毛片| 精品一区二区三区在线成人| 精品女人视频| 欧美视频一区二区三区在线观看| 中文字幕日韩一区二区三区| 99riav国产| 97精品国产综合久久久动漫日韩| 中文字幕第一区综合| 亚洲资源在线看| 欧美精品一二三四区| 91超碰在线播放| 中文字幕一区二区视频| 久久久久久草| 精品女同一区二区三区| 欧美日韩综合高清一区二区| 中文字幕在线中文字幕二区| 久久99伊人| 亚洲色图色老头| 国产清纯白嫩初高中在线观看性色| 美女被黑人40厘米进入| 亚洲视频中文| 久久久国产视频| 手机免费观看av| 免费a级人成a大片在线观看| 国产亚洲精品aa午夜观看| wwwxx欧美| 99国产精品久久久久99打野战| 国产69精品久久| 色婷婷av一区二区三区之一色屋| 国产成人一区二区三区别| 国产精品午夜剧场| 亚洲视频综合| 国外成人在线直播| 国产污视频在线看| 三上悠亚国产精品一区二区三区| 亚洲超碰精品一区二区| 97在线国产视频| 成年女人a毛片免费视频| 久久久夜夜夜| 国产精品精品一区二区三区午夜版 | 九九99久久精品在免费线bt| 精品美女调教视频| 中文字幕在线综合| 九色蝌蚪在线观看| 日韩二区在线观看| 国产精品第一视频| 国产乱码精品一区二区| 欧美久久精品| 中国人与牲禽动交精品| 精品国产精品国产精品| 日韩电影免费观| 男人天堂v视频| 99精品视频一区二区三区| 另类视频在线观看+1080p| 女人香蕉久久**毛片精品| 久久这里只有精品6| 精品日产一区2区三区黄免费| 亚洲黄色片视频| 亚洲精品亚洲人成在线| 亚洲欧美在线第一页| 日韩av片在线| bbw在线视频| 成人自拍视频网| 性欧美18+| 欧美狂欢多p性派对| 国模少妇一区二区三区| 国产精品免费在线播放| 中文字幕久热| 亚洲少妇自拍| 亚洲综合成人婷婷小说| 色精品一区二区三区| 老妇喷水一区二区三区| 国产精品三区www17con| 国产一卡2卡3卡免费网站| 日韩精品乱码av一区二区| 国产精品大全| 日本色图在线| 久久综合九色综合欧美亚洲| 亚洲自拍av在线| 97人妻精品一区二区三区软件| 亚洲欧洲美洲国产香蕉| 久久精品小视频| 怡春院在线视频| 天天做天天爱天天综合网2021| **欧美日韩vr在线| 中国女人内谢69xxxx视频|